Skip to product information
Item no. 10-464-50Sold by quote
Green Casting Alloy (10K-18K)
Price on request
Shipped across CanadaBy courier or freight: we quote delivery with your price.
Features
All the details- Green from silver#575 is made of 78.00% silver, 20.00% copper and 2.00% zinc.
- One alloy, two jobsUnited publishes separate instructions for investment casting and for making sheet, plate and wire from #575.
- Suited to enamelling#575 is a versatile alloy for enamel work.
- Softer at higher karatAs-cast hardness drops from 159 HV at 10K to 141 HV at 14K and 96 HV at 18K, by United's figures.
#575 is United Precious Metal Refining's green gold master alloy for 10K to 18K. Melt it with fine gold to cast, or pour an ingot and roll or draw it into sheet, plate and wire: United sells it as an all-purpose alloy and singles it out for enamelling. It is rich in silver (78%) and sold by weight as grain, from 50 g to 1 kg.
Casting reference by karat (United PMR data)
| Karat | Fine gold + #575, per 100 g | Casting temperature | Density | As-cast hardness |
|---|---|---|---|---|
| 10K | 41.7 g + 58.3 g | 920-940 °C (1,688-1,724 °F) | 12.48 g/cc | 159 HV |
| 14K | 58.5 g + 41.5 g | 965-985 °C (1,769-1,805 °F) | 13.89 g/cc | 141 HV |
| 18K | 75.0 g + 25.0 g | 975-995 °C (1,787-1,823 °F) | 15.65 g/cc | 96 HV |
Fine-gold weights follow standard fineness: 417 for 10K, 585 for 14K, 750 for 18K.
| Maker | United Precious Metal Refining |
|---|---|
| Product code | 575 |
| Colour | Green |
| Karat range | 10K-18K |
| Form | Alloying grain |
| Use | All-purpose: investment casting, and sheet, plate and wire |
| Composition | Silver 78.00%, copper 20.00%, zinc 2.00%, nickel 0% (published figures; United adds proprietary metals it doesn't list) |
| Pre-alloying (casting) | 1,040-1,050 °C (1,904-1,922 °F) |
| Flask temperature | 510-650 °C (950-1,202 °F) |
| Quench and remelt | Quench 8-12 minutes after casting; remelt with 50% fresh metal |
| Ingot (fabrication) | Melt at 1,050-1,060 °C (1,922-1,940 °F); pour at 1,010-1,030 °C (1,850-1,886 °F) |
| Annealing | 704 °C (1,300 °F) for 20 minutes, then quench at once |
| Sold as | By weight: 50 g, 100 g, 500 g or 1 kg |
| Made in | USA |
Sold as
By weight: 50 g, 100 g, 500 g or 1 kg of #575 alloy grain. No fine gold, flux or investment included.
Good to know
- Pouring an ingot for sheet or wire: load the alloy first and the fine gold over it in a clean crucible, melt at 1,050-1,060 °C (1,922-1,940 °F), stir well, then pour at 1,010-1,030 °C (1,850-1,886 °F) into a preheated or lightly oiled iron mould. Pour steadily and ease off at the end so the top of the ingot doesn't shrink.
- Rolling and annealing: clean oxide and flux off the ingot, then roll or draw it to half its size before each anneal. Anneal at 704 °C (1,300 °F) for 20 minutes and quench straight away, under a boric acid fire coat if you anneal in open air. Too much annealing grows the grain and leaves an orange-peel surface.
- Quench, but mind heavy ingots: an ingot goes into pickle or water as soon as it leaves the mould; give a heavy one about a minute first so it doesn't crack.
- Casting: a little boric acid flux is enough, with no carbon-based flux and none in a bottom-pour automatic caster. Invest in a gypsum-bonded investment and devest with a fluoric-based remover rather than strong acid.
- Work out the metal from the wax: multiply the alloy's density by the wax pattern's weight in grams and add 10% for the button; at 14K the density is 13.89 g/cc.
Need help choosing?Tell us what you’re making and we’ll point you to the right size and item number.