Ultra White All-Purpose Alloy (10K-18K)
Features
All the details- Casting and fabrication in one alloyUnited publishes full instructions for both, from flask temperatures to annealing schedules.
- Less nickel than our #930 and #915 casting alloys19.50% in the master alloy, against 22.00% and 30.50%.
- Hardens as the karat rises143 HV at 10K, 163 HV at 14K and 188 HV at 18K as cast, per United.
- Excellent workabilityIn United's words: it rolls and draws in 50% steps between anneals.
European Design's #862 Ultra White is United Precious Metal Refining's all-purpose master alloy for 10K to 18K white gold: the same alloy serves for lost-wax casting and for ingots rolled into sheet or drawn into wire. United describes it as low in nickel, with excellent workability. Sold by weight, 50 g to 1 kg.
Working data by karat (United PMR)
| Karat | Fine gold by weight | Casting temperature | Ingot pour (sheet, wire) | Density | Hardness as cast |
|---|---|---|---|---|---|
| 10K | 41.7% | 1,085-1,105 °C (1,985-2,021 °F) | 1,010-1,020 °C (1,850-1,868 °F) | 11.07 g/cc | 143 HV |
| 14K | 58.5% | 1,025-1,045 °C (1,877-1,913 °F) | 1,000-1,030 °C (1,832-1,886 °F) | 12.62 g/cc | 163 HV |
| 18K | 75.0% | 995-1,015 °C (1,823-1,859 °F) | 1,000-1,030 °C (1,832-1,886 °F) | 14.65 g/cc | 188 HV |
Pre-alloy at 1,090-1,100 °C (1,994-2,012 °F) for 10K, 1,050-1,060 °C (1,922-1,940 °F) for 14K-18K. For ingots, first bring the melt to 1,045-1,060 °C (1,913-1,940 °F). Flask 540-675 °C (1,004-1,247 °F); quench after 25 minutes; re-melts should be 70% fresh metal. Fine-gold percentages are standard karat fineness; the master alloy makes up the rest.
Works with
- Boric Acid Powder
- Reversible Ingot Mould Wire/Flat
- Carbon Stirring Rods
- Ceramic Casting Crucible
| Maker | United Precious Metal Refining |
|---|---|
| Alloy | 862, Ultra White, all-purpose |
| Karat range | 10K-18K |
| Use | Casting; ingots for sheet, plate and wire |
| Composition | Copper 63.50%, zinc 17.00%, nickel 19.50%, silver 0.00%, plus proprietary metals United doesn't list (nickel-based) |
| Form | Alloy grain |
| Annealing | 710 °C (1,310 °F) for 20 minutes, then cool in moving air |
| Sold as | By weight, 50 g - 1 kg |
Sold as
By weight: order 50 g, 100 g, 500 g or 1 kg (1,000 g) of alloy grain. Fine gold is not included: melt it in to reach the karat you need.
Good to know
- Casting: flux it with only a little boric acid, never a carbon flux such as soda ash or saltpetre, and use none at all in a bottom-pour automatic caster. Invest in a gypsum-bonded investment on its maker's burnout cycle, and clear the castings with a fluoric-based investment remover; a strong acid can pit the surface.
- How much metal to melt: multiply the density for your karat by the wax pattern's weight in grams, then add 10% for the button.
- Pouring an ingot: load the alloy first and the fine gold over it, stir the melt thoroughly, and pour in one steady stream into a warmed iron mould (a rod mould for wire, an L-shaped two-part mould for sheet), easing off at the end so the top of the ingot doesn't shrink. Quench straight away in pickle or water, but let a heavy ingot stand for about a minute first so it doesn't crack.
- Rolling and drawing: clean the ingot, take it down by half, anneal, clean again and repeat. Paint on a boric acid fire coat before annealing in open air, and don't over-anneal: it grows the grain and leaves an orange-peel surface.
- Don't mix it up with our other white alloys: #930 and #915 are casting alloys, and #866 is for fabrication only; #862 does both.